REPOSITORY > RESULTS

Doctoral dissertation

Investigations of the electrocaloric effect in the polycrystalline 0.9Pb(Mg1/3Nb2/3)O3-0.1PbTiO3 relaxor ferroelectric

Author(s): Marko Vrabelj (Author), Barbara Malič (Supervisor), Zdravko Kutnjak (Co-Supervisor)

Thesis defense date: 20.07.2016

Organization: MPŠ - Mednarodna podiplomska šola Jožefa Stefana

PID: 20.500.12556/ReVIS-15039

Views: 4 | Downloads: 0

Abstract

The electrocaloric (EC) effect is the change in entropy and, consequently, in temperature
of a dielectric material due to the electric-field-induced changes in the polar states. The (1-
x)Pb(Mg1/3Nb2/3)O3-xPbTiO3 (PMN-100xPT) solid solution with x≤0.35 has been widely
studied for its excellent dielectric and piezoelectric properties, and recent studies have also
shown that the compositions exhibiting the dielectric permittivity maximum close to room
temperature, such as PMN-10PT, exhibit a great potential for EC applications. Although
it has been generally accepted that the microstructure crucially influences the dielectric
properties of ferroelectric and relaxor ferroelectric ceramics, the correlations between the
microstructure and EC phenomena have not yet been explored.
We show that a substantial enhancement of the EC effect is achieved by a properly
engineered ceramic microstructure. Single-phase perovskite ceramic materials with relative
densities exceeding 95 % and with grain sizes ranging from 2.8 μm to 9.4 μm were prepared
by sintering of mechanochemically synthesized powder compacts. The largest EC
coefficient, i.e., the ratio of the EC temperature change (Δ𝑇𝐸𝐶) and electric field
amplitude, is obtained for the ceramics with 5.8-μm grains, i.e., a more than 10 % higher
value than for the materials with finer or coarser grains, as a consequence of its larger
saturation polarization. The EC response of a material is limited by its dielectric breakdown
strength, which increases with an increasing density and decreasing grain size.
For the material with an ~98 % relative density and 3.6-μm grains, the Δ𝑇𝐸𝐶 of 3.45 °C
is achieved at an electric field amplitude of 160 kV/cm. This Δ𝑇𝐸𝐶 is the highest reported
so far for Pb-based perovskites and it is comparable to the best results obtained by multicritical-
point enhancement.
The PMN-10PT ceramics with similar densities and grain sizes of ~5 μm prepared from
the powders obtained by the mechanochemical and columbite synthesis routes are
compared. Despite the very similar EC coefficients, the mechanochemically derived ceramic
displays a much larger Δ𝑇𝐸𝐶 of 2.37 °C than the columbite-derived ceramic (1.39 °C) due
to the higher dielectric breakdown strength (115 kV/cm vs. 57 kV/cm). The difference is
ascribed to different levels of chemical homogeneity and trace contaminants introduced
during the powder synthesis, which are reflected in the different domain sizes and dielectric
properties of the respective materials.
In the last part we analyze the energy-efficiency of an EC cooling system in view of the
polarization – electric field (𝑃 − 𝐸) hysteresis losses of the EC materials, and recovering
the electric energy that is consumed for inducing the EC effect (electric-energy recovery).
The energy efficiency of the materials with large hysteresis losses, i.e., PMN-100xPT
compositions close to the morphotropic phase boundary, is significantly reduced as
compared to the PMN-rich relaxor compositions. Therefore, we propose that the EC
materials with low 𝑃 − 𝐸 hysteresis losses, such as PMN-100xPT with x≤0.1, and a highdegree
of the electric-energy recovery should be implemented in an EC cooling system in
order to achieve a high energy efficiency.

Attachments

Cite this work