Views: 0 | Downloads: 0
This thesis is related to the preparation of porous Pb(Zr0.53Ti0.47)O3 ceramics using the sacrificial-template method and the patterning of Pb(Zr0.53Ti0.47)0.98Nb0.02O3 thick-film structures by inkjet printing. Porous ceramic and thick-film structures were designed for applications as backing and piezoelectric layers, respectively, in high-frequency linear-array transducers. The study consists of (i) investigation of the stability of the PZT powder in aqueous solutions at different pHs, (ii) the preparation and characterization of porous ceramics, (iii) the preparation of PZT-based suspensions, and (iv) ink-jet printing of PZT-based elements on a selected substrate.
The chemical stability of the powder with the nominal composition Pb(Zr0.53Ti0.47)O3, synthesized by solid-state synthesis at 950 °C, was studied in aqueous media at pH 3, ~3.7, 7 and 10 for 14 days. The concentrations of the Pb, Zr and Ti ions in supernatants, determined by inductively-coupled-plasma mass spectroscopy, were higher at pH 3 and 3.7 than at pH 7 and 10, while the concentration of Pb ions was higher than those of Zr and Ti, regardless of the pH. The substantial leaching of ions in acidic pHs was associated with the formation of soluble acetate complexes on the surface of the PZT. The PZT dissolved incongruently in acidic solutions, leading to a lead-deficient surface of the powder. This powder then started to densify at a 50 °C higher temperature than the as-synthesized powder and after sintering at 1050 °C the ceramic was highly porous (40 %) and contained a secondary ZrO2 phase. On the other hand, the density, dielectric and piezoelectric properties of the ceramics prepared from powders aged at pH 7 and 10 were comparable to those of the ceramics obtained from the as-synthesized powder (without aging), indicating that neutral and alkaline pHs are suitable for the preparation of suspensions.
We investigated the preparation of PZT ceramics with a tailored porosity, pore size and pore-size distribution using a sacrificial template method. Porous ceramics were prepared from the powder with the nominal composition Pb(Zr0.53Ti0.47)O3, synthesized by solid-state synthesis at 1100 °C (P1100), and spherical polymethylmetacrylate (PMMA) particles with diameters of 1.5 μm and 10 μm, which were used as templates. PMMA and P1100 particles with 0.5 wt. % polyethyleneimine (PEI) were stabilized in water at pH 7 and exhibited opposite zeta-potentials, enabling the hetero-coagulation process of both particles. After drying the suspension with P1100:PMMA in a volume ratio 70:30, both phases were homogeneously distributed in the powder mixture. The amount of porosity, the size and the shape of the pores of the ceramic sintered at 1080 °C corresponded to the volume fraction of PMMA and its initial size and shape. We thus obtained porous PZT ceramics with 30 % of porosity and interconnected ~1 μm pores or predominantly ~8 μm spherical pores depending on the PMMA particles used (1.5 m or 10 m in size).
The weak-field dielectric permittivity and piezoelectric coefficients, and the high-field polarization and the strain responses decreased with the increasing porosity and decreasing pore and grain sizes, suggesting an important role of pore/grain size on the switching behavior and sub-switching properties. The longitudinal wave velocity and the acoustic impedance of the porous ceramics were lower than that of the dense ceramics and did not depend on the pore size. In contrast, the attenuation coefficient α was shown to depend on the pore size. The α for the ceramic with ~8 μm pores was 0.96 dB (mm MHz)-1, almost three times higher than the highest reported value in the literature. The high α value obtained in this study could enable the reduction of the backing thickness and thus the overall transducer size.
In the final part of the thesis we report on the procedure for processing rectangular-shaped thick-film structures on electroded alumina substrates using piezoelectric inkjet printing. The powder with a nominal composition Pb(Zr0.53Ti0.47)0.98Nb0.02O3 was synthesized by solid-state synthesis at 1100 °C and milled in a colloidal mill. The particles were stabilized in water at pH 8 with 6 wt. % PEI and de-agglomerated by high-energy ultrasound. The final particle size dv90 of the ultrasound-treated powder was 0.42 μm, which is 50 times smaller than the nozzle size of the selected printer, and thus suitable for printing. The viscosity of the suspension was increased to 7.1 mPa·s using glycerol, while the surface tension was lowered to 30 mN/m by adding phenyl ethoxylate. The resulting ink with a Z value of 4.2 was used for printing.
The results show that the drop size increases with an increasing voltage amplitude. Shorter durations of the waveform made it possible to prevent the formation of the satellites and to improve the drop-to-drop positional accuracy. Drops without any satellites and with a good positional accuracy were obtained at the voltage amplitude of 30 V and a duration of the waveform of ~9 μs. Lines with a length of 4 mm were printed under these conditions with a drop spacing of 20 μm. The printed lines heated to 400 °C exhibited a uniform width, smooth surface, parallel side edges and a constant interspace between the lines, as evidenced by the scanning and confocal microscope analyses. We showed that by applying 2 to 5 printing drops in the Y direction we can tailor the thickness of the lines in the range from 4 μm to 7 μm, and the width of the lines in the range from 81 μm to 151 μm. The geometry of the line-shaped structures is suitable for linear-array transducers.